A practical guide to inorganic scaling, organic contamination, representative sampling, activity testing, and separating fouling from attrition or operating changes
Author: Yicarb Technical Expert (15+ years experience in activated carbon industry)
Carbon fouling in CIP and CIL occurs when unwanted inorganic or organic species accumulate on activated carbon or within its pore structure and reduce the rate or capacity of gold adsorption. A decline in gold adsorption activity does not automatically prove that the carbon is fouled: physical attrition, changes in slurry chemistry, poor mixing, altered residence time or sampling errors can produce similar plant symptoms. A reliable diagnosis combines representative carbon sampling, controlled gold-adsorption activity tests, foulant analysis and a review of operating conditions.
Activated carbon is not perfectly selective for the gold-cyanide complex. Depending on solution chemistry, it can also adsorb or accumulate other species. Technical literature on hydrometallurgical circuits describes inorganic precipitates such as calcium carbonate, calcium sulphate and silica, as well as organic compounds such as petroleum-derived oils and wood-related organics, as potential foulants that can obstruct pores and slow adsorption or elution. [1]

Figure 1: Inorganic scaling, organic contamination and mixed fouling can affect carbon in different ways.
|
Fouling category |
Potential sources / examples |
Possible effect on carbon |
|
Inorganic scaling |
CaCO₃, CaSO₄, silica / silicates, metal hydroxides or precipitates; some base-metal species may also load onto carbon |
Mineral deposits can cover external surfaces, block pore entrances or occupy adsorption space; response to acid washing depends on species and form |
|
Organic fouling |
Flotation collectors and frothers, oils, lubricants, degreasers, surfactants, humic / fulvic matter and other process-water organics |
Adsorbed organics may compete with gold species and reduce access to adsorption sites; some organic foulants require thermal reactivation |
|
Mixed fouling |
Co-deposition of mineral scale and organic matter, often with process-water and reagent contributions |
A single cleaning step may not remove all contaminants; activity recovery can be partial |
A 2011 Hydrometallurgy study found that the effect of flotation and dewatering reagents depended on reagent type and concentration. It also reported that combined effects were not simply additive and that the presence of a reagent in a continuous circuit did not always produce a harmful fouling effect. The presence of a suspected chemical is a clue, not proof of the root cause. [3]
Carbon samples must represent the operating circuit and the carbon condition being investigated. A convenient grab sample from one storage bin may not reflect the entire inventory or show where activity is being lost. Where possible, collect separately identified samples from relevant adsorption stages and from the same carbon cycle at key points such as loaded, eluted, acid-washed and regenerated carbon.
· Record the tank or circuit position, date, carbon state, sampling point and any recent process changes.
· Use a representative composite where the objective is to assess the wider inventory; retain stage-specific samples when diagnosing a local problem.
· Avoid mixing loaded, eluted, acid-washed and regenerated carbon into one sample unless the test plan specifically requires it.
· Separate carbon from slurry promptly after sampling so continued adsorption does not change the measured solution grade; filter the slurry solution promptly where solution-gold analysis is required.
A published gold-recovery technical guide recommends regular sampling across the circuit and emphasises immediate separation of carbon from slurry to prevent additional gold adsorption after sampling. It also highlights the importance of sampling records, particularly where carbon movement changes the identity of individual tanks. [2]
Carbon activity is commonly assessed by measuring how quickly a known gold-bearing solution loses dissolved gold when it contacts a defined mass of carbon. The resulting adsorption curve or rate constant is compared with a fresh-carbon control or an agreed reference carbon. This is a comparative kinetic test, not a universal pass/fail number.
· Use a defined gold solution and document its initial gold concentration and chemistry.
· Control and record pH, free cyanide, temperature, ionic strength, agitation, carbon mass, particle-size fraction and contact time.
· Take multiple time-point samples so the adsorption-rate trend can be compared, rather than relying only on one end-point result.
· Run a fresh reference carbon under the same conditions and report activity as a relative value or fitted kinetic rate parameter, where appropriate.
· Where capacity is also important, assess equilibrium or final gold loading separately from the initial adsorption rate.
Published activity-test procedures differ in equipment, solution composition, carbon concentration, particle size and pre-treatment. A classic World Gold conference paper describes a batch kinetic approach using a control carbon and expressing results as a rate constant or relative activity; the authors stress that test conditions and experimental variables must be controlled. There is no single universal ASTM method that defines every CIP/CIL gold-carbon activity test. [4] One published World Gold conference method used a three-hour batch kinetic test with several intermediate sampling points; the authors reported approximately ±10% variation in the calculated rate constant for that specific procedure. These figures describe a historical comparative method, not a universal acceptance limit or a substitute for a mine-specific protocol. [4]

Figure 2: A controlled sampling and activity-testing workflow helps separate carbon condition from plant effects.
|
Possible cause |
Typical evidence |
How to check |
|
Fouling / contamination |
Gold adsorption rate decreases; inorganic deposits or organic residues may be detected; particle-size distribution may remain broadly similar |
Compare activity before / after suitable cleaning; analyse ash, elemental deposits or organic residue where relevant |
|
Attrition / mechanical wear |
More fines and undersize carbon, visible breakage, lower retained inventory, possible decline in hardness |
Compare sieve distributions, fines generation and hardness; inspect screens, pumps, transfers and handling points |
|
Operating-condition change |
Plant extraction worsens but a controlled laboratory activity test may remain close to the fresh-carbon reference |
Review gold tenor, free cyanide, pH, temperature, pulp density, mixing, residence time, carbon concentration and interstage screens |
|
Mixed cause |
Activity loss occurs together with increased fines or significant process changes |
Combine chemical, physical and operating data; do not assign one cause from a single test |
ASTM D2862-16(2022) provides a method for measuring granular activated-carbon particle-size distribution. ASTM D3802-23 measures ball-pan hardness, but ASTM cautions that this result does not directly measure in-service resistance to degradation. These tests can support an attrition diagnosis, but they should be interpreted with actual fines and carbon-loss records. [5][6]
If the activity test confirms a loss, additional analysis can help identify what is on the carbon. Depending on the suspected material, a qualified laboratory may use ash and elemental analysis, ICP-OES or XRF for inorganic loading, and LOI / TGA, FTIR or SEM-EDS to investigate organic residues or the location and form of deposits. These are supporting analytical options rather than one mandatory test package; the method should be selected to answer a specific diagnostic question.
Compare results across the same carbon cycle. If activity improves after acid washing, an acid-soluble inorganic deposit may have been important. If improvement occurs mainly after thermal reactivation, organic foulants may have contributed. If neither step restores activity, consider mixed deposits, irreversible pore changes, carbon damage or an operating-condition problem. Diagnosing carbon fouling in CIP and CIL therefore requires comparing the carbon's activity profile with its physical condition and the plant's operating record.
· For confirmed acid-soluble inorganic scale, review the site's established acid-washing procedure and the source of scaling ions; do not assume every metal complex or deposit is removed by acid.
· For organic contamination, review reagent carryover, flotation chemicals, oil leaks, lubricants, water sources and the suitability of the thermal reactivation stage.
· For attrition, investigate carbon strength, particle-size distribution, pumps, interstage screens, agitation intensity and transfer points.
· For operating-condition changes, check solution chemistry, pulp density, gold tenor, mixing, carbon inventory and residence time before changing the carbon specification.
The distinction between acid washing and thermal regeneration is important: technical literature describes acid washing as a route for selected inorganic deposits and thermal regeneration as a route for removing adsorbed or pyrolysed organic matter. The actual sequence and conditions are plant-specific and should follow the mine's validated process and safety controls. [1][2]
Illustrative example — not a customer case study: A CIL plant observes a slower gold-loading profile and higher dissolved-gold losses. A representative sample from the regenerated-carbon stream shows lower activity than a fresh reference, while particle-size distribution and hardness remain close to historical values. The laboratory detects elevated inorganic deposits and organic residue. The team then reviews acid-wash and thermal-regeneration performance separately and checks process-water and flotation-reagent inputs. This combined evidence points toward mixed fouling rather than simple attrition or a change in operating conditions alone.
YICARB recommends monitoring carbon condition through a consistent activity profile and supporting physical and chemical checks. Testing loaded, eluted, acid-washed and regenerated carbon separately helps identify which stage is failing and avoids unnecessary fresh-carbon additions or process changes.
Carbon fouling in CIP and CIL can result from inorganic scaling, organic contamination or mixed deposits, but a loss of gold adsorption activity can also come from attrition or changing plant conditions. Representative sampling, controlled activity testing against a fresh reference, foulant characterisation and a review of operating data provide a more reliable diagnosis than any single indicator. Understanding the actual cause of carbon fouling in CIP and CIL is the basis for choosing an effective corrective action.
[1] Follis, R. H. (1992), "Assessing Activated Carbon Quality in Hydrometallurgical Circuits", SME.
[2] Rogans, "Activated Carbon in Gold Recovery", Kemix technical guide.
[3] Salarirad & Behnamfard (2011), Hydrometallurgy 109, 23–28.
[4] "CIP Carbons—Selection, Testing and Plant Monitoring", World Gold ’89 proceedings.
[5] ASTM D2862-16(2022), Particle Size Distribution of Granular Activated Carbon.
[6] ASTM D3802-23, Ball-Pan Hardness of Activated Carbon.